Sustainable Chitosan-Citric Acid Films via Homogeneous Cross- Linking: Comparative Structure−Property Analysis for Green Packaging Applications Margherita Izzi, Andrea Brattelli, Maria Chiara Sportelli,* Luigi Gentile,* Nicola Cioffi, and Rosaria Anna Picca Cite This: ACS Appl. Eng. Mater. 2026, 4, 3230−3241 Read Online ACCESS Metrics & More Article Recommendations *sı Supporting Information ABSTRACT: Sustainable chitosan-citric acid films were developed through homogeneous cross-linking, for potential application as biodegradable food packaging. Chitosan (CS) from food waste offers antimicrobial properties, but suffers from poor mechanical strength and high water affinity compared to conventional plastics. This study presents an efficient cross-linking strategy, using citric acid (CA, 2%w/v) and glycerol (Gly, 2%w/v), and comparing commercial CS with agricultural-fertilizer-grade one (biological CS). Films were characterized before/after thermal curing (150 °C, 10 min) using ATR-FTIR, WAXS, TGA, mechanical analysis, and water uptake analysis. Curing converted ionic CS-CA interactions to covalent amide bonds, reducing water uptake >90% (1027% → 94% for commercial CS; 926% → 87% for biological CS) and enhancing tensile strength while maintaining flexibility via glycerol plasticization. WAXS revealed comparable crystallinity indices (69−75%) between CS sources, confirming agricultural-grade CS viability. Cu particles incorporation (1 g/L) could impart enhanced antimicrobial functionality, without compromising mechanical performance. This homogeneous cross-linking eliminates multistep drying of heterogeneous methods, offering an environmentally friendly, scalable route to high-performance bioplastic films as petroleum plastic alternatives. KEYWORDS: chitosan, cross-linking, citric acid, SAXS, spectroscopic analysis, mechanical properties ■ INTRODUCTION During the second half of the 19th century, the scarcity of natural polymers (such as rubber) prompted an increased reliance on fossil-based feedstocks for the production of synthetic plastics. Owing to their ease of large-scale manufacturing, the global production of synthetic plastics has grown significantly up to nowadays, becoming the most widespread material around the world.1 However, this dramatic increase in plastic production and consumption has led to severe environmental pollution, and highlighted structural sustainability challenges within the chemical enter- prise. This prompted global initiatives (such as the Plastics Strategy promoted by the European Commission2 or the National Strategy to Prevent Plastic Pollution by the US Environmental Protection Agency3) that increasingly empha- sized Green Chemistry and Green Engineering principles to reduce waste,4 minimize hazards, and improve resource efficiency. Given that fossil resources are intrinsically finite and unsustainable, there is an urgent need to transition toward renewable carbon, biomass-derived feedstocks, and advanced recycling technologies that can support a circular polymer economy.5 Various approaches have already demonstrated the potential to repurpose and valorize plastic waste; however, further innovation in these technologies remains of critical importance. Notably, no single alternative can entirely replace fossil-based materials, highlighting the need for diverse plastic sources, responsible molecular design, and inherently low- impact materials. Nowadays research on materials science is focusing on the development and adoption of renewable alternatives for plastics production, such as natural polymers; their biodegradability prevents the accumulation of plastics in the environment. Among natural polymers, polysaccharides have shown considerable promise as renewable feedstocks for diverse applications.6 Chitosan (CS) is a distinctive poly- saccharide with inherent antimicrobial and antibacterial Received: March 24, 2026 Revised: May 25, 2026 Accepted: May 26, 2026 Published: June 9, 2026 Articlepubs.acs.org/acsaenm © 2026 American Chemical Society 3230 https://doi.org/10.1021/acsaenm.6c00355 ACS Appl. Eng. Mater. 2026, 4, 3230−3241 Downloaded from pubs.acs.org/aaemdr/article-pdf/4/6/3230/65232582/acsaenm.6c00355.pdf by INDIAN INST OF TECH KHARAGPUR user on 13 November 2026
properties,5,7 making it particularly attractive for niche food- related applications. However, chitosan films suffer from poor thermo-processability,8 high water affinity, and relatively weak mechanical properties9 compared to conventional plastics,10 limiting their commercial viability. To overcome these drawbacks and enhance key performance parameters such as tensile strength and water resistance,11 chemical or physical modifications are necessary, through the use of additives aligned with sustainable design criteria (e.g., renewability, low toxicity, biodegradability).12 Importantly, for environmentally responsible design, the additives used should be biodegradable as well. Inducing intermolecular cross-linking between polymer chains is one of the easiest strategies to overcome bare CS limitations.13 This approach is particularly promising due to its potential to simultaneously enhance both mechanical strength and water-resistance properties. An effective cross-linker should be Generally Recognized as Safe (GRAS),14 renewable, and capable of forming at least two covalent bonds. A wide range of cross-linking agents can be employed, including aldehydes, which form Schiff base linkages with amino groups, or genipin, a naturally derived agent known for lower cytotoxicity.15 Ionic cross-linkers like tripolyphosphate (TPP) are also widely used, enabling mild processing conditions through electrostatic interactions. Additionally, multifunctional carboxylic acids provide alternative covalent strategies with tunable cross-link density.16 The choice of cross-linker significantly influences film behavior and properties. Con- sequently, selecting an appropriate cross-linking system is essential for tailoring CS films to specific applications.17 Besides, according to the International Union of Pure and Applied Chemistry (IUPAC), plasticizers are substances added to materials (typically plastics or elastomers) to enhance their flexibility, processability, or extensibility.18 In this study, citric acid (CA) was selected as a natural cross-linking agent, and glycerol (Gly) as plasticizer. The films were prepared using the solvent casting method,19 with acetic acid serving as the solvent for chitosan. In previous chitosan - citric acid cross- linking studies, a technique referred to as heterogeneous cross- linking was commonly used, wherein the bare CS film is soaked into CA solutions.20 This approach dramatically increased preparation times, because two drying steps were required, and generally caused alterations in the original shape of the solution-cast films. Homogeneous cross-linking, instead, foresees the addition of the agent directly into the film-forming solution; in this case, although competition between citric acid and acetic acid occurs for the amidic functionalities of CS, film preparation procedures can be made much easier. After the drying step in air, films were cured in an oven at 150 °C, to foster the formation of a covalent bond between CS chains and CA molecules: this supplementary step further enhanced the mechanical and water-resistance performances of the prepared films.21 Cu particles were introduced as a model inorganic filler for enhanced antimicrobial applications.22 Cu is an essential trace element required for biological processes in plants, animals, and humans, where it functions as a cofactor in numerous enzymes.23 At low concentrations, such as those used in the composites prepared in this study, it is considered environmentally safe under European Union regulations (e.g., EU Regulation 2018/1981).24 Given the final Cu concen- tration in our composite films (1 g/L), the total metal content per square centimeter of film (∼0.6 mg of Cu/cm2) remains below the safety thresholds established by EU regulation, thus making these bioplastic films still in line with environmentally responsible design. A comprehensive multitechnique character- ization of films at each step of their preparation allowed us to investigate the cross-linking mechanism and the effect of each additive on the final material. To the best of our knowledge, this is the first study that elucidates how CA, Gly, and Cu particles influence the mechanical properties (hardness/ flexibility) and water resistance of CS films (both individually and in combination) by integrating complementary insights from multiple characterization techniques. The novelty lies not in the combination of additives itself,25,26 but in the comprehensive, multitechnique approach used to clarify the role of each additive in the final bioplastic film, with and without thermal treatment. FTIR spectroscopy was used to understand the interaction between CS and additives at a molecular level, along with thermogravimetric analysis (TGA); wide-angle X-ray scattering (WAXS) was exploited to study the possible semicrystalline nature of the films; rheological/ mechanical properties were directly correlated with the aforementioned characterizations, and with water upt
Synthesis of Cu Particles The materials and the experimental protocol adopted for the preparation of Cu particles were reported in our previous works.22,32 Briefly, 2 mM polyvinylpyrrolidone (PVP), copper sulfate pentahydrate CuSO4 * 5H2O 0.01 M, and 0.08 g/mL D-glucose were mixed and reacted at pH = 9, for 2 h, at 80 °C, as described in.22 The produced colloids were then washed and recovered as described in.32 Film Formation Purified CS (either CS_Sig or CS_Bio) was dissolved in 2%v/v acetic acid at the concentration of 2%w/v. The solvent was preheated at 50 °C, and the powder was then added gradually up to complete dissolution. The solution was kept under stirring at 50 °C for 3 h in a glass bottle. Then, the bottle was sonicated for 30 min, to eliminate gas bubbles in the solution. 2%w/v of Gly was then added under moderate stirring; after 30 min, 2%w/v CA homogeneous cross-linker was added as powder, and the mixture was let mixing for 1 h. 40 mL of the film forming solution were poured in Petri dishes (diameter: 10 cm), and dried for 18 h in a shaking incubator (10 rpm) at 35 °C. For Cu-modified samples, a 1g/L EtOH suspension of Cu particles was added 10 min before the pouring step of the film forming solution.22 Self-standing films were peeled from the Petri dishes once dried, and cured in a furnace at 150 °C for 10 min. Table 1 reports sample naming and corresponding characteristics. The total amount of Cu in the final films was measured using inductively coupled plasma-mass spectrometry (ICP-MS). A Thermo Fischer iCAP RQ was used to this aim. CA_Gly_Cu and CA_Gly_Cu_RET samples were analyzed, for both CS sources. 50 mg of film were digested using 2 mL of HNO3 65% and 6 mL of HCl 37%, and digested in a digestion apparatus (DigiPREP from QuantAnalitica) at 95 °C for 2 h. After this step, the resulting solution was filtered through 0.45 μm Teflon tubes and analyzed. Spectroscopic Characterization Chemical characterization of CS films was obtained by attenuated total reflectance Fourier transform infrared (ATR-FTIR) analysis on a Spectrum Two Spectrometer from PerkinElmer, with a resolution of 2 cm−1 and with scanning from 4000 cm−1 to 400 cm−1, on a diamond, single bounce waveguide. 32 scans were averaged; background spectra were acquired against air. Spectra were subjected to baseline subtraction and ATR correction, using the instrument software. Wide-Angle X-ray Scattering (WAXS) The WAXS pattern of the films was obtained using the SAXSpoint 2.0 instrument (Anton Paar GmbH, Graz, Austria), a Small- and Wide- Angle X-ray Scattering (SAXS/WAXS) system. The SAXSpoint 2.0 was equipped with a Primux 100 microfocus X-ray source (Cu Kα radiation, λ = 0.15418 nm, 50 W), and the scattering intensity I(q) was recorded using a Dectris EIGER R 1 M detector (Dectris Ltd., Baden, Switzerland) with a pixel size of 75 × 75 μm2. Data were acquired with the EIGER detector mounted in a tilted configuration to record the WAXS pattern (for semicrystalline materials might also be referred as X-ray diffraction pattern, XRD), covering a 2θ range from 2° to 42°. The sample temperature was maintained at 25 °C using a solid sample holder. Thermogravimetric Analysis (TGA) TGA of polymer films was performed using PerkinElmer Pyris TGA. Samples of 1−5 mg were heated from 30 °C (held for 5 min) to 600 °C (held for 5 min) in 10 °C/min steps under constant nitrogen flow (20 mL/min). The experimental data were used to plot TGA (normalized weight loss vs temperature) and the first derivative of the weight loss (DTG) curves. Tensile Mechanical Analysis The tensile mechanical analysis was performed using an Anton Paar MCR 702e equipped with a single motor. Films were cut in 1 × 5 cm2 stripes with a scalpel, and their thickness was measured with an electronic caliper, and ranged between 100 and 200 μm. To ensure that the samples were under tension during the oscillatory measurements, a preload of 0.15 N was applied to the films. In the tensile tests, the moving profile was set to apply a strain rate of 0.6 mm/min. The normal force required to maintain a constant elongation rate is measured by the instrument and converted into extensional stress values (using the geometric parameters of the loaded sample). Measurements would be stopped when the measured normal force reaches 0 N, indicating complete sample failure. All tests were conducted at 21 ± 1 °C. Statistical analysis was performed using one-way analysis of variance (ANOVA), followed by Tukey’s post hoc multiple comparison test, to evaluate differences in elongation, tensile strength, and Young’s modulus among the various samples. All data were processed using MATLAB software (MathWorks, Natick, MA, USA). A confidence level of 95% (p < 0.05) was used to determine statistical significance. Water Uptake and Water Contact Angle Measurements Water uptake measurements were conducted on samples of approximately 10 mm2, in 5 replicates, and their initial weight was measured with a 5-digit a
handling properties and elasticity, allowing for the formation of soft and pliable films even after thermal treatment. The carboxylic functionality on CA forms a stable ionic bond with the NH3+ of protonated CS, thereby obtaining a chemically cross-linked structure. This electrostatic interaction is postu- lated to become covalent (through amide bond) upon thermal treatment. CS dissolves in HAc through protonation of amine groups to NH3+, forming a soluble system governed by the acid−base equilibrium of HAc (pKa ∼ 4.76). When CA is introduced, its triprotic nature (pKa1 ∼ 3.1, pKa2 ∼ 4.7, pKa3 ∼ 6.4) increases proton availability and broadens the range of conjugate base species.34 The lower pKa1 of CA enhances CS protonation, while partially deprotonated citrate species act as multivalent counterions.35 This leads to partial replacement of acetate by citrate and formation of CS-citrate ionic pairs. Due to its trivalency, citrate can bridge multiple protonated amine sites, promoting interchain electrostatic interactions and transient physical cross-linking.36 These effects are most pronounced near pKa2, as in this study, where acetate and citrate coexist, resulting in a heterogeneous counterion environment. Overall, combining HAc with CA shifts the system from simple monovalent counterion interactions to a multivalent polyelectrolyte complexation regime.37 We esti- mated the molar ratio of reactive groups (three carboxylic groups COOH from citric acid to amine groups NH2 from CS) per 1 g of CS powder, taking into account the degree of deacetylation (DD), which determines the fraction of monomer units bearing free amine functionalities. Only the deacetylated units contribute reactive NH2 groups, making DD a key parameter in the stoichiometric evaluation. Indeed, based on the deacetylation degree (DD) values of the two types of chitosan, and molecular weights38 of glucosamine and acetylated glucosamine monomer units, the approximate ratios between aminic (NH2) functionalities and carboxylic (COOH) ones (NH2:COOH), were calculated to be 0.29 for CS_Sig and 0.33 for CS_Bio (see SI for calculations).39 Under these conditions, the number of carboxylic acid groups is around three times higher as that of the free amino groups, so the second most probable interaction that could cause cross-linking of the chitosan chains (besides amidic bond) can be either a hydrogen bond or a dipole-charge interaction.38,40 Films prepared with biological and commercial CS showed some differences, starting from visual appearance. Although both types of films appeared flat, opaque, and yellowish, the ones derived from CS_Bio were darker (Figure S1a) than the ones from CS_Sig (Figure S1b). Upon curing, a brownish color was shown (Figure S1c, d), and a more compact structure was formed. The presence of Cu in the thin films significantly altered their visual appearance, due to the brown color of the Cu particles (Figure S1e, f). The total Cu content was measured by ICP-MS on dried and cured films. For CS_Bio it was equal to 0.0043 ± 0.0013 g/L in CA_Gly_Cu, and 0.0050 ± 0.0015 g/L in CA_Gly_Cu_RET. In the case of CS_Sig, we had 0.0110 ± 0.0030 g/L in CA_Gly_Cu, and 0.0099 ± 0.0029 g/L in CA_Gly_Cu_RET. These values are lower than the nominal Cu concentration (1 g/L); this effect, typical of CS matrices, is due to the strong affinity of CS for Cu2+ ions produced upon mineralization. Amine and hydroxyl groups strongly chelate Cu2+; these coordination sites can hardly release ions even upon acidic and thermal treat- ments.41−43 Besides, the presence of a more compact polymer structure after curing enhances this effect; this results in a furtherly lower measured Cu content. Attenuated Total Reflectance Infrared Spectroscopy (ATR-FTIR) Prior to solvent casting, purified powders were analyzed and compared with the spectra of as-purchased CS (Figure S2). The purification step is effective in removing impurities, especially in the case of CS_Bio: after purification, the broad band between 3400 and 3200 cm−1 (C−H and N−H stretching) is narrowed, and the region comprised between 1620 and 1510 cm−1 (amide and carboxylic groups) becomes more pronounced. No significant differences are instead appreciated for CS_Sig, although purification ensures (in both cases) the elimination of insoluble CS fractions.27 CS films were analyzed through ATR-FTIR to gather information about intramolecular interactions between CS and additives. No significant differences were noticed between the two types of CS investigated (Figure S3). All the roto-vibrational signals relevant to a CS-based matrix were identified. The presence of additives deeply alters the spectroscopic fingerprint peaks of bare CS (Figure 1). The presence of Gly is responsible for the increased complexity of the spectral regions between 1500 and 1300 cm−1, and 1200− 900 cm−1.44 The peaks in the range 1460−1200 cm−1 and 1160−1000 cm−1 are due to C−O−H and C−O−C groups, respectively.45 The first feature
the band attributed to the O−C = O asymmetric stretching of CA,47 at ∼ 1714 cm−1,48 clearly visible in the CA_Gly films for both CS types, is no more appreciable upon thermal curing (CA_Gly_RET). This is indicative of the formation of a covalent amidic bond between CS and CA, corresponding to the typical stretching at ∼ 1640 cm−1.47 When Cu particles are present within the film, this phenomenon is partially inhibited (CA_Gly_Cu and CA_Gly_Cu_RET), due to the coordina- tion of Cu and Cu2+ ions at the aminic and hydroxyl functionalities of CS.49 As a further confirmation, C−H asymmetric group stretching and CH2 bending (amide III residues) are attributed to the feature at ∼ 1410 cm−1, clearly visible in bare CS films; this feature fades upon the addition of CA (and Gly), due to steric hindrance between CS adjacent chains.21 In the spectra of films containing Cu particles, no significant variation in the bands relevant to C−OH and C−N functionalities are visible, indicating the presence of a weak electrostatic coordination rather than a chemical bond with Cu moieties.50 Wide-Angle X-ray Scattering Wide-angle X-ray scattering (WAXS) was employed to investigate the molecular ordering and crystalline structure of the cross-linked films. The WAXS pattern (Figure 2A-D) was characterized by two scattering angles at 2θ ≈ 10° (020) and 2θ ≈ 20° (110). A third peak at 2θ ≈ 22° (120 or 200), corresponding to the allomorphic tendon form of chitosan,51,52 appeared only as a small shoulder. The tendon form, observed particularly when chitosan is cast or stretched into films, is associated with a more aligned or extended-chain crystalline structure, similar to that seen in collagen-rich tendon tissues. The 2D WAXS pattern is dominated by the amorphous halo for all samples including the one containing Cu (Figure 2E-H). The crystallinity index (CI) in percentage could be estimated by the Focher et al. method,53 which consists in applying eq 2= ×CI I I I 100am110 110 (2) where I110 is the maximum intensity at 2θ ≈ 20° corresponding to the (110) lattice diffraction, and Iam is the intensity of the amorphous region at 2θ ≈ 16°. These parameters were determined on samples before cross-linking. Tual et al. have shown that heterogeneous cross-linking does not affect the crystallinity of CS.54 In the case of homogeneous modification, Kurita et al. showed that cross-linking of CS with glutaraldehyde (GA) decreases its crystallinity at a low degree of substitution.55 Monteiro and Airoldi reached a similar conclusion for the homogeneous cross-linking with different molecules.56 In the present study, to account for the altered diffraction features of the system and the clearly detectable contribution of the (120) diffraction plane of the tendon form, the Focher method was modified by including this reflection in the crystallinity index calculation, leading to the formulation of eq 3 and providing a more representative evaluation of the crystalline fraction.= + + ×CI I I I I I ( ) ( ) 100am110 120 110 120 (3) The values of crystallinity index in Table 2 were thus obtained. The applied eq 3 provides values consistent with reported results for chitosan systems using eq 2.57 It is worth noting that the crystallinity index may be influenced by the model used for its calculation. There is no statistical difference between CS_Bio and CS_Sig in the reticulated films (CA_Gly_RET), while there is a difference between the CS_Bio and CS_Sig Figure 2. WAXS patterns for both CS_Sig (black) and CS_Bio (green): CA_Gly_RET (A), CA_Gly (B), CA_Gly_Cu (C) CA_Gly_Cu_RET (D). 2D WAXS pattern for CA_Gly_RET, CS_Bio (E), CA_Gly_RET, CS_Sig (F), CA_Gly_Cu_RET, CS_Bio (G) and CA_Gly_Cu_RET, CS_Bio (H), where gray represents the background, while blue and light blue indicate high intensity. ACS Applied Engineering Materials pubs.acs.org/acsaenm Article https://doi.org/10.1021/acsaenm.6c00355 ACS Appl. Eng. Mater. 2026, 4, 3230−3241 3234 Downloaded from pubs.acs.org/aaemdr/article-pdf/4/6/3230/65232582/acsaenm.6c00355.pdf by INDIAN INST OF TECH KHARAGPUR user on 13 November 2026
films that are not reticulated. Additionally, crystallinity increases in the presence of Cu particles. In fact, dispersed particles could facilitate the crystallization process: the high surface area of these fillers can promote faster crystallization kinetics, leading to a higher degree of overall CI, although the specific effect depends heavily on the filler loading, dispersion, and particle type.58,59 The values are in agreement with the literature.60−62 Tensile Analysis and Water Uptake Mechanical properties of thin films were evaluated by tensile testing, and the results are reported in Figure 3. The elongation at break and tensile strength are notably influenced by the presence of cross-linking, plasticizing agents, and inorganic Table 2. Crystallinity Index Values Obtained on CS Films, before and after Curing, in the Presence and Absence of Cu Particlesa CS_Sig CS_Bio CA_Gly_RET 70.1 (a) 69.8 (a) CA_Gly 74.3 (c) 71.8 (b) CA_Gly_Cu 73.4 (d) 75.1 (d) CA_Gly_Cu_RET 73.1 (d) 74.0 (c) aError is ± 0.2 for each value. Letters in the table indicate statistical significance based on the Tukey test following the ANOVA (p < 0.05) performed on the complete set of measurements. Figure 3. Tensile mechanical analysis of biological chitosan (CS_Bio: a, b, and c) and commercial chitosan (CS_Sig: d, e, and f) films under investigation: elongation at break (a and d), tensile strength (b and e), and Young’s module (c and f). Red columns refer to films dried for 18 h at 35 °C; blue columns refer to films subjected to thermal curing (150 °C, 10 min). Letters indicate statistical significance based on the Tukey’s HSD test following the ANOVA performed on the complete set of measurements. ACS Applied Engineering Materials pubs.acs.org/acsaenm Article https://doi.org/10.1021/acsaenm.6c00355 ACS Appl. Eng. Mater. 2026, 4, 3230−3241 3235 Downloaded from pubs.acs.org/aaemdr/article-pdf/4/6/3230/65232582/acsaenm.6c00355.pdf by INDIAN INST OF TECH KHARAGPUR user on 13 November 2026
species. In particular, samples dried at 35 °C exhibit values nearly twice those of thermally treated ones, indicating that mild processing conditions preserve chain mobility and result in higher deformability. The introduction of citric acid and plasticizer (CS_CA_Gly) promotes covalent cross-linking within the CS matrix, leading to a reduction in elongation at break compared to neat CS, accompanied by a decrease in tensile strength and Young’s modulus. This suggests that, under the present conditions, covalent cross-linking induces a less efficient stress transfer, possibly due to reduced chain alignment or the formation of a more heterogeneous network. The incorporation of Cu species (CS_CA_Gly_Cu) further modulates the mechanical response. Specifically, the elongation at break decreases compared to CS_CA_Gly, indicating a restriction of chain mobility due to additional coordination interactions. However, it remains higher than that of neat CS, highlighting the combined effect of plasticization and partial network flexibility. The tensile strength of CS_CA_Gly_Cu is slightly lower than that of CS_CA_Gly, although the difference is not statistically significant, and both systems exhibit lower values than neat CS. Conversely, Young’s modulus shows a slight (statistically significant) increase upon Cu addition compared to CS_CA_Gly, while remaining significantly lower than that of CS. These observations suggest that Cu moieties (Cu and Cu2+) act as physical cross-linking points through coordination with amino and hydroxyl groups of CS chains. Such interactions create additional junction zones that locally stiffen the network, explaining the slight increase in Young’s modulus. At the same time, these coordination bonds may disrupt optimal covalent cross-linking and polymer chain packing, leading to a marginal decrease in tensile strength and elongation compared to CS_CA_Gly. Although ATR-FTIR data indicate that the presence of inorganic species may partially inhibit covalent bond formation between CS and CA, the coordination-driven network introduced by Cu compensates for this effect by enhancing intermolecular cohesion. Nevertheless, this com- pensation is not sufficient to recover the mechanical perform- ance of neat CS, which likely benefits from a more homogeneous structure and higher effective load transfer. These findings are consistent with WAXS results, which show a slight decrease in the CI upon cross-linking. This suggests that the structural modifications primarily affect the amorphous regions, where both covalent and coordination interactions are established. Consequently, the mechanical behavior arises from a balance between reduced crystallinity, covalent network formation, and coordination-driven physical cross-linking. Overall, the combined presence of CA and Cu introduces a more complex network in which covalent and coordination interactions coexist, resulting in materials with intermediate stiffness, reduced strength, and higher elasticity compared to neat CS. Similar trends are observed for both dried and thermally treated films, with only minor differences attributable to processing conditions. This increased mechanical resistance after thermal treatment is directly reflected in the improved water stability of the films, as evidenced by a reduction in water uptake %. Besides the formation of a covalent bond, the instauration of Cu-mediated coordination networks densifies the polymer matrix and limits the availability of hydrophilic sites, thereby reducing water diffusion and swelling capacity. Indeed, considerable variations were observed in the ability of the CS films to sorb water (Figure 4), depending on the presence of CA and/or Cu particles, and to the performance of thermal treatment (cross-linking). The establishment of a covalent bond between CS chains and CA molecules upon thermal treatment at 150 °C is confirmed by the significant (p < 0.05) lowering of water uptake%, which goes from 926% and 1027% for uncured films of CS_Bio and CS_Sig, respectively, to 87% and 94%, respectively. The baseline value of non-cross-linked CS, ∼ 1000%, is in agreement with what reported in literature for similar films.63−65 The presence of inorganic Cu particles in the thin film does not alter this trend, and agrees with mechanical analysis and WAXS results; however, correspond- ent percentages are lowered for both types of polymer. Particles fill the spaces between polymer chains, reducing the free volume available for water molecules.66,67 Posthoc comparisons performed using Tukey’s HSD test confirmed that no significant difference was observed between the two groups of samples (CS_Bio and CS_Sig). The surface wettability, evaluated via Young−Laplace analysis of contact angle data, confirms the impact of both the chitosan source and thermal cross-linking on interfacial behavior (Figure S4). For CS_Bio_CA_Gly_Cu, the contact angle remained relatively stable after curing, shifting from 44.9 ± 0.6° i
observed after curing are consistent with the formation of a denser, more reorganized polysaccharide network. Thermogravimetric Analysis TGA and DTG data were acquired for all the thin films. DTG curves are reported in Figure 5, while corresponding TGA can be found in Figure S5. In all the curves, the initial mass loss around 120 °C corresponds to the evaporation of physically adsorbed water and other volatile components (HAc entrapped in CS network). Based on this experimental evidence, we can exclude that HAc is somehow participating in the cross-linking mechanism upon thermal treatment at 150 °C. The second degradation step, which marks the onset of structural decomposition of CS, reaches a maximum around 189 °C in all samples. This stage is attributed to the decomposition of amino- groups, and occurs at a relatively lower temperature due to the presence of glycerol.25 For dried films (Figure 5a, b) the third degradation peak, associated with the decomposition of −CH2OH groups, exhibits a maximum at approximately 240 °C (Figure 5a). The fourth degradation step is linked to the breakdown of the CS ring structure, particularly the cyclic ether moieties (around 375 °C). No substantial difference was observed between CS_Bio and CS_Sig in terms of overall degradation temperature, except for slight variations in residual water content (Figure 5a). The presence of Cu particles (Figure 5b) slightly affected the decomposition temperature. The second and third degradation steps appear to merge at lower temperatures for CS_Sig and at slightly higher temperatures for CS_Bio, whereas the fourth degradation peak consistently occurs at a lower temperature. After thermal curing (Figure 5c, d), the merging or separation of the second and third degradation steps reflects differences in polymer structure, due to covalent cross-linking and decreased chain mobility, while the fourth peak remains basically invariant, as it represents the decomposition of the more stable CS ring (Figure 5c) structure. Upon introducing Cu particles, the second and third peaks become clearly distinguishable again (Figure 5d). The reappearance of distinct degradation peaks upon Cu addition likely reflects a modification of the degradation pathway due to Cu-CS interactions and enhanced heat transfer, rather than a simple thermal stabilization or destabilization effect. This could be considered a further confirmation of the interaction of Cu and Cu2+ ions with the hydroxyl and aminic functional groups of CS with a partially inhibited covalent bond formation between CA and CS. No significant differences between CS_Sig and CS_Bio are observed, in terms of the temperature of major degradation steps. ■ CONCLUSIONS The incorporation of citric acid (CA) and glycerol (Gly), along with the implementation of a thermal curing step during film preparation, enhanced both the mechanical strength and water resistance of chitosan (CS)-based bioplastics. These mod- ifications contributed to the formation of a more robust Figure 5. DTG curves of CS_CA_Gly samples (a), CS_CA_Gly_Cu samples (b), and corresponding CS_CA_Gly_RET (c) CS_CA_Gly_Cu_RET (d). Blue curves refer to CS_Bio, and red ones to CS_Sig. ACS Applied Engineering Materials pubs.acs.org/acsaenm Article https://doi.org/10.1021/acsaenm.6c00355 ACS Appl. Eng. Mater. 2026, 4, 3230−3241 3237 Downloaded from pubs.acs.org/aaemdr/article-pdf/4/6/3230/65232582/acsaenm.6c00355.pdf by INDIAN INST OF TECH KHARAGPUR user on 13 November 2026
polymeric network, improving the material’s performance under conditions relevant to food packaging applications. Furthermore, the addition of inorganic fillers, specifically copper (Cu) particles, provided an additional reinforcement effect, further augmenting the mechanical integrity and hydrophobicity of the films. This is true although experimental evidence demonstrated the partial inhibition of a covalent amidic bond formation between CA and CS. This approach facilitates the transformation of CS into a viable alternative to conventional synthetic polymers used in the food industry. Desirable levels of water swelling and mechanical perform- ance were achieved through a controlled solvent casting process combined with homogeneous cross-linking. The presence of Gly played a key role in maintaining the flexibility and softness of the CS films, thereby enhancing their handling properties and making them suitable candidates for replacing petroleum-derived plastics. Spectroscopic and structural analyses, including ATR-FTIR and WAXS, revealed for the first time the direct correlations between the molecular structure and the macroscopic properties of the films. These findings provided insight into the cross-linking mechanisms, and confirmed the uniform distribution of the fillers and cross- linking agents within the polymer matrix. Additionally, the influence of different CS sources was evaluated, comparing CS derived from biological origin (CS_Bio) with commercially available CS (CS_Sig). The results demonstrated comparable mechanical properties between the two, suggesting that the proposed fabrication strategy is broadly applicable regardless of CS origin. Overall, the methodology presented herein offers a promising route for the development of green, sustainable, and biodegradable bioproducts derived from chitosan. The comparison between the films here proposed and what is already present in literature demonstrates: (i) substantially lower water uptake (down to ∼ 87−94%) compared with many reported CS-based films, which often display swelling values several hundred percent higher;68 (ii) improved balance between tensile strength and flexibility due to the optimized CA/Gly combination;69 (iii) comparable crystallinity indices and thermal stability despite the use of low-cost biological CS;70 (iv) a simpler and more scalable preparation route based on homogeneous cross-linking and single-step curing.20 These considerations strengthen the positioning of the present work within the current state of the art and clarify its contribution toward scalable, sustainable food-packaging bioplastics. Compared with previously reported similar CS-based films, the present materials combine low swelling behavior, preserved flexibility upon inorganic filler inclusion, scalable homogeneous processing, and the successful use of low-cost biological CS feedstocks, representing a significant advancement toward industrially viable green packaging materials. These materials have the potential to replace nonbiodegradable synthetic polymers currently in widespread use, contributing to the advancement of environmentally responsible technologies in the packaging sector. ■ ASSOCIATED CONTENT Data Availability Statement The data that support the findings of this study are freely available upon request to the Corresponding Authors. *sı Supporting Information The Supporting Information is available free of charge at https://pubs.acs.org/doi/10.1021/acsaenm.6c00355. Visual appearance of CS-based films; Calculation of the approximate ratios between aminic (NH2) function- alities from chitosan, and carboxylic (COOH) ones from citric acid; ATR-FTIR of CS powders; ATR-FTIR spectra of CS-based films; contact angle measurements for the chitosan-based composite films; TGA curves (PDF) ■ AUTHOR INFORMATION Corresponding Authors Maria Chiara Sportelli − Chemistry Department, University of Bari Aldo Moro, Bari 70126, Italy; Center of Colloid and Surface Science (CSGI) - Bari, University of Bari Aldo Moro, Bari 70126, Italy; Institute for Photonics and Nanotechnologies, National Research Council (IFN-CNR), Bari 70126, Italy; orcid.org/0000-0002-8832-2770; Email: maria.sportelli@uniba.it Luigi Gentile − Chemistry Department, University of Bari Aldo Moro, Bari 70126, Italy; Center of Colloid and Surface Science (CSGI) - Bari, University of Bari Aldo Moro, Bari 70126, Italy; orcid.org/0000-0001-6854-2963; Email: luigi.gentile@uniba.it Authors Margherita Izzi − Chemistry Department, University of Bari Aldo Moro, Bari 70126, Italy; Center of Colloid and Surface Science (CSGI) - Bari, University of Bari Aldo Moro, Bari 70126, Italy; Institute for Photonics and Nanotechnologies, National Research Council (IFN-CNR), Bari 70126, Italy; orcid.org/0000-0001-5158-2352 Andrea Brattelli − Chemistry Department, University of Bari Aldo Moro, Bari 70126, Italy; Center of Colloid and Surface Science (CSGI) - Bari, University of Bari Aldo Moro, Bari 70126, Italy Nicola Ci
Funding L.G. was funded by the Italian Ministry of University and Research (MUR) under the program Italian Science Fund (FIS 2021), Starting Grant (number FIS00003259). Notes The authors declare no competing financial interest. ■ ACKNOWLEDGMENTS Mr. Michele Amoia and Ms. Alessia De Cataldo are acknowledged for their help in acquiring experimental data. ■ REFERENCES (1) European Environmental Agency. Plastics. European Environ- mental Agency. https://www.eea.europa.eu/en/topics/in-depth/ plastics. (2) European Commission. Plastics strategy. https://environment.ec. europa.eu/strategy/plastics-strategy_en. (3) US EPA. National Strategy to Prevent Plastic Pollution. US Environmental Protection Agency. https://www.epa.gov/ circulareconomy/national-strategy-prevent-plastic-pollution (accessed 2026−02−16). (4) Gururani, P.; Bhatnagar, P.; Dogra, P.; Chandra Joshi, H.; Chauhan, P. K.; Vlaskin, M. S.; Chandra Joshi, N.; Kurbatova, A.; Irina, A.; Kumar, V. Bio-Based Food Packaging Materials: A Sustainable and Holistic Approach for Cleaner Environment- a Review. Current Research in Green and Sustainable Chemistry 2023, 7, 100384. (5) Nguyen, M. T. P.; Escribà -Gelonch, M.; Hessel, V.; Coad, B. R. A Review of the Current and Future Prospects for Producing Bioplastic Films Made from Starch and Chitosan. ACS Sustainable Chem. Eng. 2024, 12 (5), 1750−1768. (6) Janik, W.; Jakubski, Ł.; Kudła, S.; Dudek, G. Modified Polysaccharides for Food Packaging Applications: A Review. Int. J. Biol. Macromol. 2024, 258, 128916. (7) Chandarana, C.; Bonde, S.; Sonwane, S.; Prajapati, B. Chitosan- Based Packaging: Leading Sustainable Advancements in the Food Industry. Polym. Bull. 2025, 82 (11), 5431−5462. (8) Fernández-Marín, R.; Morales, A.; Erdocia, X.; Iturrondobeitia, M.; Labidi, J.; Lizundia, E. Chitosan-Chitin Nanocrystal Films from Lobster and Spider Crab: Properties and Environmental Sustain- ability. ACS Sustainable Chem. Eng. 2024, 12 (28), 10363−10375. (9) Blilid, S.; Kędzierska, M.; Miłowska, K.; Wroń ska, N.; El Achaby, M.; Katir, N.; Belamie, E.; Alonso, B.; Lisowska, K.; Lahcini, M.; Bryszewska, M.; El Kadib, A. Phosphorylated Micro- and Nano- cellulose-Filled Chitosan Nanocomposites as Fully Sustainable, Biologically Active Bioplastics. ACS Sustainable Chem. Eng. 2020, 8 (50), 18354−18365. (10) Khankhuean, A.; Morimura, Y.; Ajiro, H. Improving the Mechanical Properties of Chitosan through Blending with Poly- (Trimethylene Carbonate) Copolymer. Int. J. Biol. Macromol. 2024, 283, 137830. (11) Tancredi, M.; Carandente Coscia, C.; Buonocore, M.; Cangiano, A.; Salvatore, M. M.; Veronico, L.; Picone, D.; D’Ursi, A. M.; Grimaldi, M.; Ottaviani, M. F.; Guido, S.; Paduano, L.; Gentile, L.; D’Errico, G. Concentrated Rhamnolipid Formulations: Bridging Chemodiversity to Structure, Flow Behavior, and Functionality. ACS Sustainable Chem. Eng. 2026, 14 (1), 415−427. (12) Lu, Z.-L.; Xing, Y.-Z.; Zheng, W.-S.; Han, Y.; Zhang, Z.-Y.; Wang, J.; Liu, C.-G. Hydrogen-Bonding Cross-Linking Agent- Reinforced Chitosan/Cellulose Composite Films for Fresh Fruit Preservation: An Experimental and Theoretical Study. ACS Sustainable Chem. Eng. 2025, 13 (27), 10597−10610. (13) Guerrero, P.; Muxika, A.; Zarandona, I.; de la Caba, K. Crosslinking of Chitosan Films Processed by Compression Molding. Carbohydr. Polym. 2019, 206, 820−826. (14) FOOD AND DRUG ADMINISTRATION. GRAS Substances (SCOGS) Database. FDA. https://www.fda.gov/food/generally- recognized-safe-gras/gras-substances-scogs-database (accessed 2026−02−16). (15) Kildeeva, N. R.; Privar, Yu. O.; Bratskaya, S. Yu. Crosslinking Agents in the Targeted Design of Chitosan-Based Materials. Colloid J. 2025, 87 (6), 875−902. (16) Lewandowska, K. Influence of Cross-Linking Agents on the Structure and Stability of Chitosan and Carboxymethyl Chitosan Thin Films. Molecules 2026, 31 (2), 272. (17) Woźniak, A.; Biernat, M. Methods for Crosslinking and Stabilization of Chitosan Structures for Potential Medical Applica- tions. J. Bioact. Compat. Polym. 2022, 37, 151. (18) Vieira, M. G. A.; da Silva, M. A.; dos Santos, L. O.; Beppu, M. M. Natural-Based Plasticizers and Biopolymer Films: A Review. Eur. Polym. J. 2011, 47 (3), 254−263. (19) Siemann, U. Solvent Cast Technology - a Versatile Tool for Thin Film Production. In Scattering Methods and the Properties of Polymer Materials; Stribeck, N., Smarsly, B., Eds.; Springer: Berlin, Heidelberg, 2005; pp 1−14. DOI: 10.1007/b107336. (20) Shu, X. Z.; Zhu, K. J.; Song, W. Novel pH-Sensitive Citrate Cross-Linked Chitosan Film for Drug Controlled Release. Int. J. Pharm. 2001, 212 (1), 19−28. (21) Schnabl, K. B.; Mandemaker, L. D. B.; Ganjkhanlou, Y.; Vollmer, I.; Weckhuysen, B. M. Green Additives in Chitosan-Based Bioplastic Films: Long-Term Stability Assessment and Aging Effects. ChemSusChem 2024, 17 (13), No. e202301426. (22) d’Agostino, D.; Sportelli, M. C.; Gentile, L.; Desopo, M.; Izzi, M.; Incerti, O.; Sanzani, S. M.; Cioffi, N. Green Cu Particles for Functional an
(32) Sportelli, M. C.; Picca, R. A.; Izzi, M.; Cioffi, N. Green Synthesis and Analytical Characterization of Core-Shell Copper Sub- Microparticles. Chem.�Eur. J. 2023, 29 (20), No. e202203510. (33) Kukushkina, E. A.; Duarte, A. C.; Tartaro, G.; Sportelli, M. C.; Di Franco, C.; Fernández, L.; García, P.; Picca, R. A.; Cioffi, N. Self- Standing Bioinspired Polymer Films Doped with Ultrafine Silver Nanoparticles as Innovative Antimicrobial Material. International Journal of Molecular Sciences 2022, 23 (24), 15818. (34) Li, K.; Yang, X.; Dong, X.; Cao, H.; Zhuang, S.; Gu, X. Easy Regulation of Chitosan-Based Hydrogel Microstructure with Citric Acid as an Efficient Buffer. Carbohydr. Polym. 2023, 300, 120258. (35) Arpa, M. D.; Erim, Ü . C.; Salik, E. E. K.; Kaleli, S. N. B.; Erol, I. Effect of Organic Acid Selection on the Physicochemical Properties, Bioadhesion, and Stability of Chitosan Hydrogels. Gels 2025, 11 (10), 778. (36) Vo, T. S.; Chit, P. P.; Hoang, T.; Hoang, V. H.; Dang, T.-N. T.; Vo, T. T. B. C.; Park, Y.; Kim, K. Chitosan Solubility in Organic Acid Solutions under Ultrasonication: A Comparative Perspective. Int. J. Biol. Macromol. 2025, 331, 148394. (37) Chattopadhyay, K.; Xavier, K. A. M.; Ngasotter, S.; Karmakar, S.; Balange, A.; Nayak, B. B. Chitosan Gel Prepared with Citric Acid as the Food Acidulant: Effect of the Chitosan Concentration and Gel pH on Physicochemical and Functional Properties of Fish Protein Emulsion Sausages. ACS Omega 2023, 8 (8), 7829−7837. (38) Yang, G.; Lam, E.; Moores, A. Controlled Chitosan Molecular Weight Reduction by Mechanochemical and Aging-Based Phosphoric Acid Hydrolysis. ACS Sustainable Chem. Eng. 2023, 11 (20), 7765− 7774. (39) Khouri, J. Chitosan Edible Films Crosslinked by Citric Acid. Dissertation, University of Waterloo, 2019. (40) Mü nstermann, N.; Weichold, O. On the Conditions Determining the Formation of Self-Crosslinking Chitosan Hydrogels with Carboxylic Acids. Gels 2025, 11 (5), 333. (41) Yang, Z.; Chai, Y.; Zeng, L.; Gao, Z.; Zhang, J.; Ji, H. Efficient Removal of Copper Ion from Wastewater Using a Stable Chitosan Gel Material. Molecules 2019, 24 (23), 4205. (42) Rhazi, M.; Desbriè res, J.; Tolaimate, A.; Rinaudo, M.; Vottero, P.; Alagui, A. Contribution to the Study of the Complexation of Copper by Chitosan and Oligomers. Polymer 2002, 43 (4), 1267− 1276. (43) Limchoowong, N.; Sricharoen, P.; Techawongstien, S.; Chanthai, S. Using Bio-Dispersive Solution of Chitosan for Green Dispersive Liquid-Liquid Microextraction of Trace Amounts of Cu(II) in Edible Oils Prior to Analysis by ICP-OES. Food Chem. 2017, 230, 398−404. (44) Habuka, A.; Yamada, T.; Nakashima, S. Interactions of Glycerol, Diglycerol, and Water Studied Using Attenuated Total Reflection Infrared Spectroscopy. Appl. Spectrosc. 2020, 74, 767. (45) Jiang, S.; Qiao, C.; Liu, R.; Liu, Q.; Xu, J.; Yao, J. Structure and Properties of Citric Acid Cross-Linked Chitosan/Poly(Vinyl Alcohol) Composite Films for Food Packaging Applications. Carbohydr. Polym. 2023, 312, 120842. (46) Sharmin, N.; Rosnes, J. T.; Prabhu, L.; Böcker, U.; Sivertsvik, M. Effect of Citric Acid Cross Linking on the Mechanical, Rheological and Barrier Properties of Chitosan. Molecules 2022, 27 (16), 5118. (47) Nataraj, D.; Sakkara, S.; Meghwal, M.; Reddy, N. Crosslinked Chitosan Films with Controllable Properties for Commercial Applications. Int. J. Biol. Macromol. 2018, 120, 1256−1264. (48) Azeredo, H. M. C.; Morrugares-Carmona, R.; Wellner, N.; Cross, K.; Bajka, B.; Waldron, K. W. Development of Pectin Films with Pomegranate Juice and Citric Acid. Food Chem. 2016, 198, 101− 106. (49) Ilnicka, A.; Walczyk, M.; Lukaszewicz, J. P. The Fungicidal Properties of the Carbon Materials Obtained from Chitin and Chitosan Promoted by Copper Salts. Materials Science and Engineer- ing: C 2015, 52, 31−36. (50) Udoetok, I. A.; Karoyo, A. H.; Mohamed, M. H.; Wilson, L. D. Chitosan Biocomposites with Variable Cross-Linking and Copper- Doping for Enhanced Phosphate Removal. Molecules 2024, 29 (2), 445. (51) Podgorbunskikh, E.; Kuskov, T.; Rychkov, D.; Lomovskii, O.; Bychkov, A. Mechanical Amorphization of Chitosan with Different Molecular Weights. Polymers 2022, 14 (20), 4438. (52) Okuyama, K.; Noguchi, K.; Hanafusa, Y.; Osawa, K.; Ogawa, K. Structural Study of Anhydrous Tendon Chitosan Obtained via Chitosan/Acetic Acid Complex. Int. J. Biol. Macromol. 1999, 26 (4), 285−293. (53) Focher, B.; Naggi, A.; Torri, G.; Cosani, A.; Terbojevich, M. Chitosans from Euphausia Superba: Characterization of Solid State Structure. Carbohydr. Polym. 1992, 18 (1), 43−49. (54) Tual, C.; Espuche, E.; Escoubes, M.; Domard, A. Transport Properties of Chitosan Membranes: Influence of Crosslinking. J. Polym. Sci., Part B: Polym. Phys. 2000, 38 (11), 1521−1529. (55) Kurita, K.; Yoshida, A.; Koyama, Y. Studies on Chitin: New Polysaccharide/Polypeptide Hybrid Materials Based on Chitin and Poly(.Gamma.-Methyl L-Glutamate). Macromolecules 1988, 21 (6), 1579−1583. (56)
(70) Wang, L.; Ma, J.; Zhang, X.; He, S.; Duan, Y. Preparation and Characterization of Chitosan/Citric Acid Composite Film and Its Application in Blueberry Preservation. Carbohydr. Res. 2026, 559, 109714. ACS Applied Engineering Materials pubs.acs.org/acsaenm Article https://doi.org/10.1021/acsaenm.6c00355 ACS Appl. Eng. Mater. 2026, 4, 3230−3241 3241 Downloaded from pubs.acs.org/aaemdr/article-pdf/4/6/3230/65232582/acsaenm.6c00355.pdf by INDIAN INST OF TECH KHARAGPUR user on 13 November 2026